Wound dressing nanofibers: PCL and HA scaffold data

A polymer solution pulled through an electric field becomes a nonwoven mat of submicron filaments, and that is the whole reason wound dressing nanofibers get attention from formulation groups. The fiber diameter lands near the scale of natural extracellular matrix fibrils, and the surface area packed into each milligram is large. A 2026 in vitro study ran six PCL based compositions through morphology, wetting, tensile testing, fibroblast viability, scratch closure, and disc diffusion, then set out in plain terms what the numbers could not support. The second half is as instructive as the first.

Quick answer. Of the six wound dressing nanofibers tested, the composition built from 10% PCL, 0.5% HA, and 1% standardized Cotinus coggygria leaf extract was the only one that held fibroblast viability above 80% across the full 0.062 to 1 mg/mL range. It also produced the highest tensile strength at 2.40 +/- 0.15 MPa and the highest elongation at break at 178 +/- 18%. Wetting behavior followed the extract rather than the HA. Antibacterial performance followed neither: the widest inhibition zone belonged to the mat with no HA and no extract, which the authors put down to residual processing solvent. No release testing, no measured loading, and no animal work were done, so what the paper describes is a workable scaffold, not a validated delivery system.

Why PCL and hyaluronic acid belong in the same fiber

PCL degrades slowly and holds its shape in a moist environment, which is what a dressing needs, but it is hydrophobic and biologically quiet. The PCL-only mat here wet out at 122 +/- 3 degrees, and that number is the inertness written as an angle. Water gathers instead of spreading. HA brings the opposite set of properties: it is hydrophilic, it gives cells something to attach to and multiply on, and it carries anti-inflammatory signaling through receptor mediated pathways. What it does not bring is strength or persistence, since it hydrates and disperses long before a dressing interval ends.

The pairing divides the labor. Polyester carries the mechanical load so the mat survives being cut, lifted, and pressed onto a wound, while HA handles the interface with tissue. Geometry contributes a third thing: far more surface per milligram than a film of equal mass, which serves both fluid uptake and the release of anything loaded into the fiber.

How the six wound dressing nanofibers were built

Every concentration was given as percent weight per volume of the total solvent, so the lead recipe of 10% PCL, 0.5% HA, and 1% extract equals 1.00 g PCL, 50 mg HA, and 100 mg extract in 10 mL of solvent. Molecular weights were 80 kDa for the PCL and 400 kDa for the HA, both picked with spinning in mind. The extract arrived as a commercial standardized material specified at not less than 30.0% total polyphenols as catechin, 15.0% flavonoids as apigenin, 2.0% flavonoids as quercetin, and 32.0% tannic compounds as tannin, all on a dry basis.

The solvent choice deserves attention from anyone trying to repeat this. HA will not dissolve in acetone or DMF and will not hydrate without water, so the three HA free recipes (F1, F3, F4) were spun from acetone and DMF at 5:5 by volume, while the three HA containing recipes (F2, F5, F6) required acetone, DMF, and water at 5:4:1. Mixing happened immediately before spinning to head off phase separation. Conditions were 23 kV, a feed rate of 0.8 to 1.0 mL/h, a tip to collector distance of 10 to 12 cm, and 5 to 6 hours per batch.

FormulationComposition (% w/v)Mean fiber diameter (nm)Beads
F110% PCL390 +/- 33Numerous
F210% PCL + 0.5% HA481 +/- 27Absent
F310% PCL + 1% extract420 +/- 22Absent
F410% PCL + 3% extract635 +/- 68Absent
F510% PCL + 0.5% HA + 1% extract548 +/- 41Absent
F610% PCL + 0.5% HA + 3% extract593 +/- 48Absent

Fiber diameter and the disappearance of beads

Mean diameters for the six mats sat between 390 and 635 nm, all of them continuous submicron fibers. HA raised fiber thickness significantly in the blank group and in the 1% extract group (P < 0.05). The extract alone, added to the blank, moved diameter by no significant amount. HA together with extract pushed diameter well above the PCL-only baseline (P < 0.05). The PCL-only mat was also the only one carrying numerous beads, and beading vanished as soon as HA and extract joined the recipe.

That matters beyond appearance. Beads signal incomplete solvent evaporation or too little chain entanglement while the jet is in flight, and a beaded fiber has a cross section that changes along its length. A mat built from such fibers is weaker and scatters its mechanical measurements, so the smooth composite fibers are a real advantage of the formulation rather than a cosmetic one.

Wettability followed extract content, not hyaluronic acid

The wetting results run against the obvious guess. Half a percent of HA moved the angle from 122 +/- 3 degrees to 118 +/- 1, four degrees in total. The extract moved it about seventy: 51.5 +/- 8.5 degrees at 1% extract without HA, and 19.6 +/- 5.5 degrees at 3%. With HA in the recipe the trend was unchanged, at 65.3 +/- 3.3 degrees for the 1% extract composition, and at 3% extract the droplet was taken up completely within 3 seconds. The authors conclude that surface wettability was governed by extract content rather than by HA.

Read practically, a minor component by mass can set the surface energy of a composite mat, and a hydrophilic polymer at low loading is an unreliable route to a wettable surface. Both directions carry a cost. A dressing needs enough wetting to pull exudate in rather than leave it pooled on top, yet a mat that drinks water on contact can over-hydrate the bed and fall apart. The lead composition lands mid-range on the measured scale, which is the part of the range a working dressing would choose.

Mechanical profile: strength and stretch in one mat

The lead composition posted the highest tensile strength at 2.40 +/- 0.15 MPa, the highest elongation at break at 178 +/- 18%, and the tightest spread of the six. The PCL-only mat managed 0.388 +/- 0.078 MPa and 38.3 +/- 19.3% elongation, while 0.5% HA on its own gave 0.945 +/- 0.081 MPa with 29.0 +/- 9.8%. At 1% extract without HA the values were 2.16 +/- 0.23 MPa and 53.8 +/- 5.2%; at 3% extract without HA they fell to 1.01 +/- 0.49 MPa and 61.5 +/- 12.7%.

The 3% extract with HA composition gave 1.70 +/- 1.03 MPa and 99.9 +/- 56.6% elongation, but the authors attach a measurement caveat: areal density varied visibly across that mat, so specimens from different regions differed in effective cross section and the means should be read as indicative. The caveat carries its own lesson. Strength and stretch normally pull against each other, since a mat stiff enough to resist a tear is usually a mat that will not drape, and the opposite holds too. The lead composition broke that trade in vitro. A separate core-shell design reinforced with mineral particles reached roughly 7.8 MPa, which places 2.40 MPa as a balance point rather than a limit.

FormulationContact angle (degrees)Tensile strength (MPa)Elongation at break (%)
F1122 +/- 30.388 +/- 0.07838.3 +/- 19.3
F2118 +/- 10.945 +/- 0.08129.0 +/- 9.8
F351.5 +/- 8.52.16 +/- 0.2353.8 +/- 5.2
F419.6 +/- 5.51.01 +/- 0.4961.5 +/- 12.7
F565.3 +/- 3.32.40 +/- 0.15178 +/- 18
F6Fully absorbed in 3 s1.70 +/- 1.0399.9 +/- 56.6

Cytocompatibility in fibroblasts: a narrow window

For wound dressing nanofibers the useful question is not whether the raw polymer is toxic but whether the finished mat is tolerated at a dose that also does something. Testing used L929 mouse fibroblasts, the line named in device cytotoxicity guidance, with the candid note that it is an immortalized subcutaneous connective-tissue line and no stand-in for the cell mix of human dermis. Medium extracts of each mat were applied at 1, 0.5, 0.25, 0.125, and 0.062 mg/mL for 24 hours. Medium alone served as the negative control at 100% viability, and 20% DMSO as the positive control at 35 +/- 2.4%.

Only the lead composition stayed above 80% across the entire ladder: 80.4 +/- 3.8% at 1 mg/mL, 92.4 +/- 1.1% at 0.5, 97.8 +/- 1.3% at 0.25, then 105 +/- 3% and 109 +/- 1% at the two lowest doses. The PCL-only mat dropped to 44.9 +/- 2.1% at the top dose. Extract effects went biphasic. At 1% loading, viability at 1 mg/mL beat the PCL-only fiber, 71.8 +/- 2.5% against 44.9 +/- 2.1%. At 3% loading it collapsed to 33.1 +/- 1.1%, and the 3% extract with HA composition fell to 58 +/- 2% at the same dose.

Double staining at 1 mg/mL reproduced the pattern. The lead composition gave 6 +/- 1% apoptotic and 10 +/- 1% necrotic cells, while the 3% extract without HA gave 21 +/- 1% and 39 +/- 3%. Necrosis outran apoptosis in every sample, and the authors read that as death inflicted by the material rather than a planned death process. HA lowered both indices wherever it appeared alongside extract. One spectral detail is worth carrying forward: in the lead composition the infrared and calorimetric traces showed PCL bands only, because PCL dominated the mass and the HA and extract features were invisible. A mat that is loaded and a mat that is shown to be loaded are different claims.

Scratch closure and the antibacterial comparison

Fibroblasts seeded at 2 x 10^5 cells/mL were scratched and followed for 24 hours. Closure reached 71 +/- 3% for the HA-only composition, 58 +/- 2% for the PCL-only mat, 57 +/- 3% for the lead composition, 47 +/- 2% for 1% extract without HA, 39 +/- 2% for 3% extract with HA, and 24 +/- 3% for 3% extract without HA, against 9.5 +/- 3.2% in the untreated control. Every formulation beat the control at both 12 and 24 hours, and higher extract loading meant less closure, matching the viability data. The authors are explicit that closure mixes migration with proliferation, since no proliferation control was run.

Disc diffusion used 30 microliters of 1 mg/mL formulation solution per disc, 24 hours at 37 degrees, with erythromycin on each plate as the comparator, against Staphylococcus aureus and Escherichia coli. On S. aureus the PCL-only mat reached 27 +/- 1 mm, the one result indistinguishable from its plate’s erythromycin disc at 28 +/- 1 mm. The lead composition reached 21 +/- 0 mm. The remaining extract containing mats reached 20 +/- 0, 15 +/- 2, 9 +/- 1, and 11 +/- 1 mm, every one of them significantly below erythromycin (P < 0.05). E. coli zones never exceeded 8 mm for any mat. The authors attribute the surprising strength of the plain PCL mat to solvent left behind by the process, and residual solvent was never measured.

Why F5 is the lead and F4 is the warning

Across the six wound dressing nanofibers, the lead composition wins on balance rather than on any single record. It is not the most wettable, not the strongest in absolute terms, and not the most antibacterial. What it alone does is stay cytocompatible down the whole concentration ladder while sitting mid-range on mechanics and mid-range on wetting. That is the profile a dressing has to hold through handling, cutting, placement, exudate contact, and days of cell contact.

The 3% extract composition without HA is the counterexample. At 1 mg/mL it was the most cytotoxic, it carried the highest necrotic index, it closed the scratch assay least, and it produced the smallest S. aureus zone. More bioactive material purchased less tolerance and less activity at the same time. The dose response here is non-monotonic, so any group raising an active loading should map viability across a ladder instead of assuming the effect keeps its direction.

Twelve limitations worth naming before scale up

  1. Solvent system and two process parameters vary alongside composition across the six recipes, so the differences observed belong to the fabrication condition as a whole and not to composition alone.
  2. Biological work used medium extracts of the mats, not intact mats against cells, so the geometry of the intended use was never reproduced.
  3. Scratch closure covers migration plus proliferation, and no proliferation control was run.
  4. The widest zone came from the mat with no HA and no extract, so zone size cannot stand in for the extract contribution.
  5. No animal model was used and every endpoint is an in vitro surrogate for healing.
  6. Sterilization effects and storage stability went untested.
  7. No release study was run, so nothing here shows controlled or sustained release.
  8. Extract content and loading efficiency were never measured, which leaves loading as a theoretical number derived from the recipe.
  9. Without an extract-only control, the extract share of cytocompatibility, closure, and antibacterial activity cannot be separated.
  10. Residual solvent was not quantified by gas chromatography and no solvent-only or vehicle disc was run, so the plain mat’s activity has no assigned cause.
  11. The cytotoxicity work fell short of the ISO 10993-5 protocol: extraction at 1 mg/mL sits below the mass-to-volume ratio specified for irregularly shaped materials, and neither material nor vehicle controls were included.
  12. The extract is a commercial standardized material checked for polyphenols and flavonoids but lacking a full chromatographic fingerprint, so batch variation cannot be ruled out.

What this means for rifamycin and other local delivery programs

For a rifamycin program the transferable content is methodological rather than clinical, and the first item is the solvent system. Bringing HA into the recipe forced a move from a two component acetone and DMF mix to a three component system containing water, because HA neither dissolves nor hydrates without it. A rifamycin loaded version of the same architecture meets the same question head on: does the compound stay soluble and stable in an aqueous containing system, and does fiber morphology survive the change. Rifampicin, rifapentine, and rifaximin differ in solubility and stability, and none of that transfers from a two solvent process.

The second item is the loading claim. Loading here is theoretical throughout, with no measured extract content and no release profile, and the limitations say so outright. For a high value active such as a rifamycin, the gap between theoretical and measured loading separates a formulation idea from a product specification, and release kinetics are what turn a loaded mat into a local delivery claim. Fiber images plus viability curves demonstrate a scaffold, not a delivery system.

The third item is the shape of the dose response. The 3% extract recipes show that raising the active fraction can flip cytocompatibility and cut the functional readout at once, and the unexplained antibacterial activity of the plain polymer mat shows why empty-mat and solvent-only controls are not optional when an antibacterial effect is claimed for a loaded dressing. Route also fixes the claim. A locally acting rifamycin whose value depends on staying where it is placed needs measured release and measured tissue exposure, not a zone diameter standing in for both. None of this argues against the architecture. It argues for testing the right things in the right order.

Bottom line

The six wound dressing nanofibers answer a narrow question cleanly. A PCL and HA mat can be spun into clean submicron fibers, loaded with a standardized polyphenol rich extract, carried through handling without tearing, and kept cytocompatible at 1% extract with 0.5% HA. They leave the question most programs actually care about untouched: how much active is in the fiber, how fast it leaves, and whether the released dose does anything in tissue. Wetting tracked the extract, mechanics peaked at one composition, and antibacterial activity tracked neither. The lead composition is a defensible place to start and a poor place to stop.

FAQ

What are wound dressing nanofibers

Wound dressing nanofibers are nonwoven mats of continuous polymer filaments with submicron diameters, made by electrospinning a polymer solution in an electric field. The fiber scale sits close to natural extracellular matrix fibrils and the surface area per unit mass is high. The six mats in this study measured 390 to 635 nm in mean fiber diameter and could take up fluid and conform to an irregular bed.

What did the lead formulation contain

The lead formulation combined 10% PCL with 0.5% hyaluronic acid and 1% of a standardized Cotinus coggygria leaf extract, all expressed as weight per volume. The PCL was 80 kDa and the hyaluronic acid 400 kDa. Spinning used 23 kV with a feed rate of 0.8 to 1.0 mL/h and a tip to collector distance of 10 to 12 cm over 5 to 6 hours.

Why did hyaluronic acid barely change the contact angle

Adding 0.5% hyaluronic acid alone moved the water contact angle only from 122 to 118 degrees. The extract moved it far more, to 51.5 degrees at 1% and 19.6 degrees at 3%. The study therefore concludes that surface wettability was governed by extract content rather than by hyaluronic acid, even though the polymer itself is strongly hydrophilic.

How were the fibers produced

All six formulations were electrospun at 23 kV with a feed rate of 0.8 to 1.0 mL/h and a tip to collector distance of 10 to 12 cm, over 5 to 6 hours. Hyaluronic acid free recipes used acetone and DMF at 5:5 by volume. Recipes containing hyaluronic acid needed acetone, DMF, and water at 5:4:1 because the polymer does not hydrate without water.

What tensile strength did the lead formulation reach

The lead formulation reached a tensile strength of 2.40 +/- 0.15 MPa with an elongation at break of 178 +/- 18%, the highest of the six compositions on both measures and with the lowest variability. The PCL-only mat reached 0.388 +/- 0.078 MPa. For scale, a separate reinforced core-shell design reported about 7.8 MPa, so 2.40 MPa is a balance point rather than a ceiling.

Which formulation was cytotoxic

The 3% extract composition without hyaluronic acid was clearly cytotoxic, with viability of 33.1 +/- 1.1% at 1 mg/mL and apoptotic and necrotic indices of 21 +/- 1% and 39 +/- 3%. The PCL-only mat fell to 44.9% and the 3% extract composition with hyaluronic acid to 58% at the same dose. Only the lead composition stayed above 80% across the whole ladder.

Did the plant extract improve antibacterial activity

Not in any way the data can support. The largest zone against Staphylococcus aureus came from the mat with neither hyaluronic acid nor extract, at 27 +/- 1 mm, which the authors attribute to residual processing solvent. Every extract containing mat was significantly less active than erythromycin, and zones against Escherichia coli stayed at 6 to 8 mm for all six mats.

What did the scratch assay show

Closure at 24 hours reached 71 +/- 3% for the hyaluronic acid only mat, 57 +/- 3% for the lead composition, and 24 +/- 3% for the 3% extract without hyaluronic acid, against 9.5 +/- 3.2% untreated. All formulations beat control. Increasing extract concentration reduced closure, and no proliferation control was applied, so the assay reflects migration and proliferation together.

Was release of the extract measured

No release test was performed, so the study provides no evidence of controlled or sustained release. The extract content in the fibers was never measured and is reported only as the theoretical value calculated from the recipe. Loading efficiency was not determined, and no extract-only control was included in the biological assays, so the extract contribution cannot be isolated.

What should a rifamycin program take from this

Three things. The solvent system had to change once hyaluronic acid entered the recipe, so a rifampicin, rifapentine, or rifaximin version would need solubility and stability re-established. Loading was never measured, so actual content and release kinetics would have to be added before any delivery claim. And the dose response was non-monotonic, so viability needs mapping across a ladder.

What should be tested before scale up

The study names the gaps itself: sterilization effects and storage stability, an in vivo model, residual solvent by gas chromatography, measured extract content and loading efficiency, release kinetics, intact mats in contact with cells rather than medium extracts, an extract-only control, a proliferation control in the scratch assay, and a full chromatographic fingerprint of the extract.

What cell line was used for cytocompatibility

Viability was measured on L929 mouse fibroblasts, the reference line recommended for cytotoxicity testing of medical devices, at five concentrations from 0.062 to 1 mg/mL over 24 hours. The study notes that this is an immortalized subcutaneous connective-tissue line and not a model of human dermis, so the results indicate cytotoxicity rather than a formal biocompatibility rating.